- Problems with Hydroxy-apatite relate to its mechanical properties and the lack of information relating to its long term effect in the body
- Delamination will occur if the layer is too thick or there are too many pores
- The ideal thickness is between 50 and 100 micron, and probably between 70 and 80 micron
- Materials testing of components with 50 micron HA coating results in no delamination after 10 million cycles
- Vacuum spraying of the coating results in a more even and less porous coating and there is less transformation to the more soluble tricalcium phosphate (TCP) as lower temperatures are required
- Need consistent solubility/stability of the coating, if it is to be used as a prosthetic surface coating
- Bonding of HA to prosthesis is due to mechanical interference and is weaker than that of other metallic porous coatings to metal. Adding a precoating of Ti on Co/Cr increases the bonding strength but adds another interface and potential site of failure
- HA should not be used on a smooth surface as it fails in shear
- Should always have a macro-lock system of component in bone as well as micro-lock of HA on prosthesis
- If the HA is going to be resorbed in the long term will give secondary fixation (70% remains in dogs after 4 months and reported 90% remains in humans after 4 years)
- Should it be placed on a porous coating ?
- Bone ingrowth into a metallic porous coating is in the order of 10 – 15%, with a HA coated prosthesis this improves to ~ 65% with the best insertion techniques
- Weight bearing results in about 200 – 500 micron movement in well sized and inserted cementless prosthesis. No ingrowth of bone will occur with movement greater than 150 micron resulting in the formation of a fibrous membrane on porous coated implants
- Experimental work from Europe suggests HA stimulates formation of fibrocartilage arranged in a radial fashion from the prosthesis which can go on to form bone in the presence of this degree of movement (animal study results)
- HA crystals released from the coating have been seen in the joint and can stimulate an inflammatory response but does also reduce the number of metallic particles released from the surface of the prosthesis
- Porous coated implants fail at a rate of 0.5% per year. Therefore, you need a study series of 3000 hips followed for at least 5 years to show that HA coated implants are better than what is currently available
Ideal make-up of HA coating
- Consistent and predictable in composition and behaviour
- 95% pure HA (not too much TCP or solubility)
- 70% crystalline (also affects solubility)